Not very scientific. I used to help make the stuff so this stuck in my mind.
I think it was Chicago and I remember it was the offices of a steel company.
It was reported that when the air pollution was reduced the rust washed off
the Corten and stained the footwalk brown.
Peter Hutchison
----- Original Message -----
From: "Kinder, Joachim" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Monday, February 23, 2009 1:37 PM
Subject: AW: Weathering steel (Cor-ten) conservation.
Dear Arantza,
as metallurgist I did a tiny bibliographic research in the past mainly to
receive information about the reason of Cor-ten steel to be more or less
corrosion-resistant. From that little research I remember that during the
formation of rust on the surface of a corroding steel the alloyed Cu will
form a subsurface-layer below the rust because of its noble character.
Problematic are surfaces of sculptures etc. which are oriented horizontally.
In this case for example rain water will pond for a while and this leads to
a penetration of the Cu-layer thereby promoting corrosion. Because this
bibliographic research happens in the early 90ties I do not have the old
results available.
Some years ago I conducted a scientific research regarding the cleaning of
old metallic surfaces which were formed during manufacturing (i.e. casting
skulls on cast iron and hammer scale on steels). The cleaning experiments
were done by the German company Kaercher (see: www.karcher.com) with
blasting techniques using high water pressure or high-pressure dry-ice
particles. Both techniques were able to clean the rusted and somewhat dirty
surface of the testing specimen sufficiently without affecting the old oxide
surface layer too much. But of course the rust was fully removed which
definitely will not be your intention!
I can provide you with a little publication about my cleaning examination
which was prepared for an international conference in Slovakia in 2006 in
English language if you like. Perhaps it might be possible to do some
examinations together with Kaercher but this time on dirty Cor-ten steel
surfaces in order to find-out proper parameters for cleaning such rust
surface without removing the wanted rusty surface too much ...
Kind regards!
Dr. Joachim Kinder
Materialprüfungsanstalt Universität Stuttgart
- Materials Testing Institute of University Stuttgart -
(MPA Stuttgart - Otto-Graf-Institut (FMPA))
Department 52350 - Failure Analysis in Mechanical Engineering
Pfaffenwaldring 32
D-70569 Stuttgart
Phone: +49 (0) 711 685-6 03 11
Fax: +49 (0) 711 685-6 39 01
e-mail: [log in to unmask]
Internet: http://www.mpa.uni-stuttgart.de
-----Ursprüngliche Nachricht-----
Von: Arch-Metals Group [mailto:[log in to unmask]] Im Auftrag von
Arantza Garcia
Gesendet: Donnerstag, 19. Februar 2009 09:06
An: [log in to unmask]
Betreff: Re: Weathering steel (Cor-ten) conservation.
Hello,
Thank you very much for the bibliography suggestion.
It is a pity it is in German. I will try to get someone to translate the
contents.
Thanks!
best
Arantza García
Dpto. de Conservación
Museo Guggenheim BILBAO
Tel: 00. 34. (9) 403 91 26 / Fax: 00.34.(9) 435 90 61
e-mail: [log in to unmask]
-----Mensaje original-----
De: Arch-Metals Group [mailto:[log in to unmask]] En nombre de
[log in to unmask]
Enviado el: jueves, 19 de febrero de 2009 8:57
Para: [log in to unmask]
Asunto: Re: Weathering steel (Cor-ten) conservation.
here is a topic about this:
http://www.nextroom.at/publication_preview.php?picture_id=463&publication_id=799&box1_id=-1#annex
> Hello all,
>
> I would like to get in contact with professionals dealing with
> conservation and
> maintenance of weathering steel (Cor-ten steel) sculptures or
> structures
> (exhibited indoors and/or outdoors).
>
> We are currently carrying out research into the deterioration and
> conservation
> of weathering steel (Cor-ten) sculptures. An area of specific
> interest in the
> project is the problem of graffiti, (protective treatments and their
> removal)
>
> Any suggestions would be greatly appreciated.
> Thanks
>
> Best
> Arantza.
Mezu honek eta eranskinek informazio konfidentziala eduki dezakete. Igorri
zaion pertsonari bakarrik zuzendua da. Legeak mezuak daukan informazioa
zabaltzea, kopiatzea edo hirugarren bati helaraztea debekatzen du. Internet
bidez bidalitako posta elektronikoak ez du konfidentzialtasuna bermatzen,
ezta transmisio zuzena ere. Mezu honetan adierazitako iritziak egilearenak
dira eta ez dute zertan bat etorri Guggenheim Bilbao Museoaren
Fundaziokoekin. Horregatik erakundeak ez du onartzen azaldutako
informazioaren gaineko erantzukizunik.
Este mensaje y sus anexos pueden contener información confidencial y están
exclusivamente dirigidos a sus destinatarios, quedando prohibida su
divulgación, copia o distribución a terceros. Si ha recibido este mensaje
por error, por favor, notifíquelo inmediatamente al remitente y bórrelo de
su sistema. El correo electrónico vía Internet no permite garantizar ni la
confidencialidad de los mensajes ni su correcta transmisión. Las opiniones
expresadas en este mensaje son las de su autor y no necesariamente las de la
Fundación del Museo Guggenheim Bilbao que no se responsabiliza de su
contenido.
This message and any attachments may contain privileged and confidential
information and are intended solely for the use of the person or entity to
whom the message was addressed, any dissemination, distribution, or use of
the contents of this message being strictly prohibited. If you receive this
message in error, please delete it and immediately notify the sender. Email
transmission cannot be guaranteed to be secure or error-free. Please note
that any opinions expressed in this e-mail are those of the author
personally and do not necessarily represent the position of the Fundación
del Museo Guggenheim Bilbao, who does not accept responsibility for the
contents of the message.
|